Friday, February 14, 2014

Smoothing Up the Left Rear Quarter


At last, the Night Mission project has reached a point where actual formal bodywork can begin!  In my last update, the left rear quarter metal work was completed and preparations were being made to begin the careful process of applying fillers and leveling all of the repaired areas. 
In most “collision” repair shops, the filling process is often a single step process before primer and paint.  Most of what drives this technique is pure profitability in a cut-throat and murderously competitive market where insurance claims dominate the landscape and any technique to shorten the turnover rate equals serious dollars on the bottom line.

The obvious down side to this is that repairs are rarely of the quality that is expected at the level “we” are looking for, and the incentive to “cave-it-and-pave-it” gets higher as the day and project progresses.  This is why I maintain my personal philosophy that shops doing everyday collision work (a.k.a. “body shops”), do not make good places to take your restoration work to.  It is an entirely different mindset.
In my shop, I hold filling a panel as essentially a three step process:  1) “Heavy” filler work which involves conventional poly filler like All-Metal and Rage, 2) “Light” filler work which centers around glazing putty with very thin applications, and finally 3) “Finish” filler work which is exclusively a sprayable, high-build filler over the entire panel that will be blocked to the perfect finish before primer/sealer application and paint.  This is obviously only a fraction of the true work involved in getting a panel flat and laser straight, but as the specifics of applying fillers goes, that is the process I follow and will document here.

On the heels of the last update where the metal work was completed and all remaining surface repairs were made, it was finally time to begin the “heavy” filler work on the quarter.  I should point out that when I use the term “heavy”, I am only referring to the density of the filler used first and NOT the amount of filler applied.  Remember, this ain’t no “body shop”.
There is a lot of opinion swirling around about whether or not to apply filler to bare metal or over an epoxy primer as a best practice.  I am of the opinion that “heavy” fillers should be applied to properly prepared bare metal surfaces for maximum adhesion.  My main reason for this is that I prefer to use a fairly aggressive sanding grit to prepare the bare metal surface that simply cannot be supported by any epoxy primer.  I like to use a DA sander with 36 grit paper to lightly scuff the bare metal surfaces in a non-directional pattern to give the fillers plenty of “tooth” to grip and hold on to.  Once the heavy filling work is complete, I seal the entire panel with epoxy and apply subsequent filling work over the primed surface after sanding with 80 grit.  This is plenty of tooth for the lighter glazing fillers and sprayable poly fillers to bond to without concern for finish integrity.  Following that, the sanding prep before the final primer/sealer coats is straight out of the preparation recommendations of the primer manufacturer and rarely gets more aggressive than 150 grit to ensure sanding marks do not surface in the upper finishing coats.

As described above, I prepared the bare metal surfaces with a light application of 36 grit paper on my DA sander, followed by a thorough washing of the surface with acetone to remove any remaining traces of marking ink or machinist dye.  Then I followed up with a thorough swabbing of the panel with commercial wax and grease remover and let everything dry thoroughly.
The first order of business is to apply a “base” filler over the areas where welds and/or heat has been applied to the panel.  I prefer to use a metalized filler called All-Metal as a base filler over these particular areas as it is extremely durable and strong and seals the welded areas extremely well.  The down side is that this material is designed to replace lead filler and this makes it much tougher to sand and shape, so I use it sparingly and NEVER as a final finish coat.

In similar fashion to the bare metal work described in my last post, I use a guide coat to act as my road map to sanding each and every coat of filler that is applied.  I prefer a graphite powdered guide coat by 3M that goes on very smooth and does an excellent job coating the entire surface of the filler evenly.  It doesn’t load the sand paper at all and is as easy to apply as wiping steam off a bathroom mirror.  It is pretty much the state of the art in guide coats and is far more economical that the old rattle can guide coat sprays of the past.
Once the All Metal filler completely covers the welded or heated areas and has been dressed down with 80 grit paper by hand below final surface, I move to my favorite “heavy” body filler called Rage Gold by Evercoat.  I have been using Rage for over 20 years and the stuff continues to perform extremely well.  Every improvement to the formula has been excellent and it has outstanding workability and sanding characteristics.  The one “trick” I employ is to shake Rage thoroughly in my pneumatic shaker rather than stirring it before use.  This removes 99% of the air bubbles in the product and gives it a buttery smooth texture that is very easy to mix and apply with virtually no pinholes.

At this point, you must condition yourself to the idea that filer work is an iterative process.  In other words, any repair area will receive several thin coats of filler, followed by DA and hand sanding between each coat until the surface is exactly as you want it.  Applying a heavy coat of filler will only create more work for you in the long run and exhaust and frustrate you during the hand blocking process.  This is an exercise in patience and discipline and it is worth taking your time to apply and finish correctly.  Since most of the filler will end up on the ground, wasting it by applying too much of it is just costing you money that could be better spent on other things.
Since I was fortunate in being able to bring the base metal very close to final shape, none of the areas I needed to fill would require very much material to get where it needed to be.  However, even the thinnest filled sections required at least 2 thin applications of filler to get the surface I was looking for.  Most areas will regularly see 4 to 6 applications depending on the amount of filler required and the complexity of the repair surface.  That is simply what it takes to get the surfaces to shape up the way they are intended without tremendous waste.

As the filler surfaces approach their final desired finish, I try to purposely slow down in my block sanding to ensure I don’t over do it.  Also, I prefer to use the longest sanding blocks possible for the area that I am working to help distribute the sanding load over the largest surface area to reduce the likelihood of plowing an edge or gouging an otherwise finished surface.
I try to discipline myself to always wear nitrile examination gloves while I sand and check the surface.  Most obviously, a glove keep the oils from my hands off the surfaces as much as possible and the thin membrane of nitrile rubber actually increases the sensitivity in the fingers, allowing very tiny irregularities to be felt in the surface that cannot be seen with the eye.

After a several days dedicated to the filling and blocking process, I had the left rear quarter panel in pretty good shape and ready to begin the prep work to get it in a thin coat of epoxy primer/sealer before moving on to the right side quarter and tail light panel.  This coat of epoxy will be the first real opportunity to see how the surfaces are shaping up and will give a hint on where the lighter filler work will be required.  Yep……we’ll be back here again before it’s over!

I prefer to cover any areas that have been welded or have heat applied as part of metal work with All-Metal filler to seal the area and provide a strong base.  I use this metalized filler sparingly as it is much more difficult to sand and shape than conventional filler.  This is a very thin skim coat, the bulk of which will be sanded away.
After sanding with a DA and blocking by hand, the All-Metal filler is in place and this area is ready for a follow-up skim of Rage Gold polyester filler to bring up the surface to the perfect finish.

One of the more heavily welded areas was this section of the quarter at the rocker joint.  I welded this seam up and smoothed it for aesthetic reasons and this is the first coat of All-Metal.

With most of the first coat of All-Metal sanded away, I use a pencil to mark the areas that will require additional filler on the subsequent coats.  Once the entire weld seam is sealed with All-Metal, I move on to Rage Gold to finish the "heavy" filler work in this area.
My favorite way to prepare Rage Gold filler for use is to shake it in my pneumatic paint shaker for 3-4 minutes.  This does an excellent job of removing air bubbles and smoothing the mixture to a perfect consistency for ease of application.  I just scoop out the desired amount, add hardener and mix it well for about a minute and go to work.  Life is not complete without a paint shaker!

While this looks like a lot of filler at first glance, it is actually a thin coat over a large area extending well beyond the actual repair areas.  This allows efficient filling of the repair while allowing blocking with the longest blocks that can be used in each area.  This makes for a much more consistent finish in shorter time than applying heavy layers and having to carve off massive amounts of cured filler before you ever get near the desired shape.

Once the Rage Gold filler "gels up", I use a Surform (a.k.a. cheese grater) file tool to shave the filler into it's rough shape.  Once this is done, the filler is left to cure fully before block sanding begins.

Here is the same area after the second coat of Rage has been blocked.  Plenty left to do, but the idea is to sneak up on the surface you want.

A third and fourth application were required before I felt the surface was where it needed to be.
A fifth and sixth filling iteration was required in the area of the lower front fender opening to get the contour just right.  After this was blocked by hand, it was time to move on to the next repair area further back on the quarter.

Very, very thin coats of filler were used in the center of the panel to get these very slight irregularities corrected.  It looks a bit daunting, but all but one of these areas was invisible to the eye and were only revealed using 3M dry guide coat as an indicator of the surface along with a hand gloved with a nitrile examination glove.  This guide coat coupled with the amplified tactile sensitivity offered by the thin nitrile glove allowed me to feel irregularities that could not be easily seen (if at all).

Here is an area that is often overlooked in custom and restored cars:  The fender lip reveal.  I take extra care to make this lip reveal even all the way around the wheel opening and to smooth it up so it blends smoothly into the fender.  It's a small detail that makes a difference people will notice subconsciously.

With All-Metal filler already applied to the roof seam, this area will be smoothed up with Rage Gold until this critical contour on the Boss is seamless and perfect before paint.

My car was originally fitted with rear window louvers.  However, they were stolen off the car in about 1977 and the damaged latch holes were all that was left.  I don't care for these louvers and long ago decided to leave them out of this build.  With that, I welded up the holes and now it has come time to apply a skim of filler over the repair area which can be seen about 1/3 of the way across the bottom of the window opening (in the middle of the sanded bare metal area).  At the same time, I will be filling the outer panel seam that was previously welded and smoothed, again for aesthetic reasons.


 
There you have it.  Though it doesn't look like much, the left rear quarter is now ready for primer/sealer and at least two more passes of filling and smoothing work yet to come.  Like I said before:  This ain't no body shop job.......

At this angle, you can better see the detail in the roof seam that is now much smoother than it was before the "heavy" filling process was complete.  You can also get an idea of just how little filling was required overall across the entire quarter.  No bad after 44 years of abuse and neglect.

Monday, February 10, 2014

Dent Repair & Metal Finishing on Left Rear Quarter

With the snowiest winter in decades demanding more time than it deserves (thank the Lord for a new snow blower!), a week of time spent out of the country for work, and a shop heater misbehaving, I was getting a bit anxious to spend proper time in the shop dedicated to the Boss since my last update.  However, though I have been delinquent in keeping up with fresh entries for a few weeks, I have managed to make good progress.

To begin, the task of repairing 44 years’ worth of accumulated dents and dings in the left rear quarter had finally come on the menu.  Having managed to clean and preserve the bare metal panel successfully, the time to sit down to the careful and particularly delicate work of dent removal and metal finishing was at hand.

After several hours of careful study of every inch of the panel, I decided it best to start at the front and top half of the quarter and methodically work my way to the back, repairing every irregularity in a given area before moving on to the front lower half and repeating the process.  This method allowed me to maintain a clear focus on each repair area until the repairs were as good as I could possibly make them.
Beginning in the area just behind the striker post, I had a nice, sharp dent that slightly deformed the leading edge and radiated back into the open panel by several inches.  Like with any proper metal work, some form of “indicator” is required to understand and visualize the extent of the damaged area so you know exactly what needs to be repaired and how far out from the heaviest damage to begin the correction.  The first rule of dent removal is to understand that dents must be removed in the reverse order in which they were created.  In other words, the outer peripheral damage must be slowly moved back into shape first if you are to get the “core” damage to move as well.  In simplest terms, if the dent started at the front and ended at the back, the repair of that dent starts at the back and moves to the front.

My preferred “indicator” on bare metal is a giant Sharpie marker instead of conventional guide coat paint.  It dries quicker, is much thinner, very easy to clean up and does a nice job of highlighting the low spots.  Oh, and it’s ridiculously cheap too!  So, the first order of business is to swab the entire repair area with Sharpie and lightly scuff the surface with a rigid sanding block with 80 grit paper.  Very quickly, the true extent of the dent is revealed and the road map for repair is defined.
Starting at the outer edge of the dent, began the repair by welding a series of draw pins about ½” inboard of the edge of the dent and began the careful process of pulling the metal while gently tapping the outer crown with a dinging spoon.  Then I cut the pins off and ground the heads smooth and inked the area.  After the ink dried, I lightly sanded the surface again with the rigid sanding block to check progress and define what area would need attention next.  This basic process was iterated about a dozen times over several hours to bring the surface as close to the original contour as possible.  Once complete, all that remained were two small shallow points where I had to shrink the metal with heat to pull the leading edge back into form and a few shadow outlines where the welded draw pins were removed.  All told, the final skim of filler that would be required will be less that about .020”.

Moving back on the quarter to the trailing fender lip radius, I had to attend to a dent that was an alarmingly similar to the first one.  Fortunately, the damage was not as severe or deep, so less time was required to get the metal to return to its original position.  Using the same technique as previously described, this dent was pulled and the fender lip radius restored such that almost no filler will be required at all.
The final metal finishing task on this quarter panel involved straightening up the area where the marker light was filled with a welded patch as an aesthetic improvement.  Since this would involve a much larger area that would require attention, I marked out the zone with a marker to help keep my mind focused on the specific repair area.  Then I coated the area with machinist dye as an indicator similar to the Sharpie marker I used earlier.  Machinist dye is easier to apply over a large area than Shaprie marker, so I use it for the sake of convenience.  Another advantage to it is that it stays wet longer and allows you to look at the panel from various angles with a high gloss on the surface to see in great detail very subtle (and not-so-subtle) irregularities in the metal that will require attention.

Again, the repair area was sanded to provide the appropriate contrast and I went to work with more conventional hammers and dollies, dinging spoons, bulls eye picks, a large shrinking disc and rubber mallets to nudge the surfaces as close as possible to the original contour.  No welded draw pins were required in this critical area.  Unfortunately, I failed to properly document this operation but I am happy to report that this are too will require very little filler to get straight.
The final area of concern was the front lower joint between the quarter and the rocker.  This area required extensive repair for rust and other damage and I welded the seam and ground it smooth for aesthetics.  Careful metal work during the reconstructive phase allowed that no heavy dent repair was required in this area as the areas that I wanted to be low (e.g. weld seams) were already in shape and the rest of the contours were very close to what they were originally.  So after a few minutes with a dinging spoon and dolly, the area was ready for filler.

With that, the “heavy” metal work on the left rear quarter was complete and it was time to plan the process of applying fillers and smoothing up the panel and the associated seams before sealing everything up with primer.

Using a huge Sharpie marker, I coat the entire damaged area and use it as a guide coat to see just where I need to work.  The camera flash already makes the dent very obvious.

Lightly sanding over the inked area very clearly shows the extent of the repair area.  As you can see in this shot, the low spot carries out into the panel quite a bit farther than can be detected with the naked eye.  However, with this technique, our work area is cleanly defined.

Beginning about 1/2" from the outer edge of the dent, I weld draw pins to the surface and begin the gentle pull-and-tap technique to ease the metal back into its original shape.  This is an iterative process that requires patience and a clear understanding that the dent must be removed in the reverse order that it was created.  In this case, the initial impact point is at the far left edge of the dent.  That is why the repair is started from the far right side as it was the "last" area to be damaged in this singular impact.

After about three hours and 32 draw pins later, the metal is almost perfectly returned to it's original form.  The two dark spots on the left edge are the result of some very localized heat-shrinking I needed to do to get the door opening edge to come back to shape.  This was done with a special tip on the stud welder gun that pinpoints the heat in a very small area and minimizes distortion in the material.  These small marks are actually very shallow, but filled with ink, so they look very pronounced in the shot.

A handful of draw pins and one less dent!

Even sky lighting the repair area shows very little filler will be required to get this area perfectly smooth.  Now to repeat this repair procedure for all of the other areas on this quarter!

My photo-documentation skills really suffered on this blog update, but the sanded area in this shot was once the location of another nasty little dent that deformed the wheel arch.  Using the identical techniques described above to remove the first dent, this area will require virtually no filler as well.

A larger and more challenging area to straighten is the rear quarter section where the original marker light hole was welded up.  To enable me to more clearly focus on the area, I outline the full extent of the work surface with a marker as seen here.

Since the repair area is much larger, I use sprayable machinist dye to coat the surface as my guide coat.  While it is wet and glossy, I can easily spot areas that will need work.  This is something I do quite regularly and often use simple wax and grease remover sprayed on the panel to check my progress and visualize the surface in final finish.  Works great!
After several hours of very gentle manipulation from both sides of the panel, the marker light area is quite straight and ready for filler.
 
The last area I needed to evaluate was the lower front joint area where the quarter and rocker join.  I welded this seam up for aesthetic purposes and repairs were required to the rocker and wheel arch area as part of the rust repair procedures.  Fortunately, the repair techniques I used allowed the welds to be slightly below the original surfaces and only slight correction to the surfaces were required before moving on.

Saturday, January 18, 2014

Removing Surface Rust & a Tip on Exposing and Eliminating Micro-Rust

When we left off last week, I had managed to get both rear quarter panels stripped to bare metal and I shared some detail on the extent of the surface rust that was hidden under the original paint that was exposed during stripping.

In this update, I have set out to remove most of the lighter surface rust with my angle grinder fitted with a surface conditioning disc.  These open-weave nylon abrasive discs make quick work or removing light rust and surface imperfections without damaging the parent metal.  Fortunately, the vast majority of the surface rust was easily removed in this way, but it also revealed a few concerns where the heavier rust deposits were.

Close inspection after cleaning up the visible rust revealed an area of tiny pits (and a few slightly larger ones) that appeared to have cleaned up.  However, experience has taught me that surface conditioning discs do not clean rust from pits very well and in all likelihood, there was plenty of microscopic rust (a.k.a. micro-rust) still living at the bottom of these tiny pits.  The problem is if you can’t see the rust, how do you eliminate it?
To many, the quick and easy answer is to haul out the sand blasting rig and assault the panel with high-velocity abrasive to remove this miniscule rust residue at the expense of all of the good metal around the areas.  Unfortunately, this is analogous to driving finishing nails with a sledge hammer.  It’s kinda the right idea, but the execution is never what you really had in mind.  However, the most effective solution to address this problem is actually simpler and cheaper than you might think.  Stay with me now……

As I have outlined many times in previous blog entries, I use a phosphoric acid Prep & Etch solution to treat and preserve all of the bare metal that is exposed while I work.  This serves many useful purposes, not the least of which is keeping flash rust in check and arresting the progression of existing rust by converting it to black ferric phosphate (FePO4) until it can be properly dealt with.  The problem here is that once the exposed surface of the rust is converted, the conversion reaction stops and the underlying rust, while essentially arrested and sealed, is still there.
But hold on a minute and let’s think about this.  If we have taken our time to prepare a nice, clean, bare steel panel by removing all traces of original paint, brushing the visible rust off the surface with a surface conditioning abrasive, sanding the surfaces smooth, and finally applying a light coat of phosphoric acid prep to preserve the panel, what more can be done to positively identify micro-rust and how do we eliminate it effectively without tearing up a perfectly viable panel?

The answer is almost ridiculously simple.  Remember how the phosphoric acid converts the rust it contacts into a black inert byproduct (ferric phosphate)?  Well why not use this very reactive characteristic as a chemical “indicator” of every spot on the clean panel that retains rust?  In other words, the black byproduct has now become a very effective and relatively high-contrast “developer” that will highlight every spot where micro-rust remains.  So, by using a phosphoric acid prep solution on your clean steel panel, you will have created a virtual “road map” of sorts that clearly shows you all of the areas that will require addition cleaning methods to remove the remaining rust.
Now that the “secret” of exposing the remaining micro-rust areas has been identified, the process of removal can begin.  This is where the process becomes a bit of a throwback to the popular sand blasting method but on a much smaller scale.  Since blasting is so effective at removing rust and other surface coatings, I have come to love a product from Zendex called the Speed Blaster along with their add-on accessory the Hot Spot abrasive recovery fixture.  Essentially, this combination creates a small, virtually dust-free miniature sand blasting apparatus that will blast small, dime-sized circles of metal with high precision and effectiveness and it only requires a few minutes to master.  By using this tool to blast each and every black “freckle” indicated by the phosphoric acid solution, I can very methodically remove even the tiniest traces of rust from pits that are almost invisible to the naked eye.  And the beautiful part is the method of checking progress is to simply reapply the phosphoric acid solution to the freshly blasted area and look to see if the black spots reappear.  If any black traces remain, I simply fire the Speed Blaster back up and repeat the process until all traces of micro-rust have been eliminated.

Once the job is complete, I treat the entire panel one final time with a phosphoric acid wash applied by hand, allowed to sit for a few minutes to etch the metal surface evenly, and then wipe off the residue with clean cloths and quickly hit the entire surface with compressed air to drive off the moisture as quickly as possible.  At this point, the panel is preserved and can be worked extensively in preparation for dent removal, fabrication work, metal finishing, and structural and cosmetic filler work.  Yep, that’s where we are heading next!

Using a surface conditioning disc on my angle grinder, I was able to remove most of the surface rust spots that were exposed once the quarter panel was completely stripped to bare metal.

I knew the surface conditioning discs would not remove the micro-rust in the tiny pits that were revealed where the heavier rust was.  I use phosphoric Prep & Etch as an indicator of where this nearly invisible rust remained so I could remove it.
To keep the phosphoric acid from getting everywhere, I use a folded paper towel to keep the acid localized in the area I am trying to treat.

Looking closely, you will see the phosphoric acid has turned the micro-rust black and it shows up quite easily against the shiny bare metal.

Now that the micro-rust can be easily seen, I can confidently remove it.  a bonus is that the phosphoric acid will continue to perform its "indicator" role for as long as necessary until I am able to remove ALL of the hidden rust.

A quick run over the entire panel with an 80 grit disc in the DA sander polishes up the metal surface nicely and adds contrast to the areas that we have treated with phosphoric.

This is a dandy tool called a Speed Blaster that allows small-scale sand blasting in your shot without making a mess.  With the proper rubber nozzle on the Hot Spot recovery unit, you can sand blast dime-sized spots wherever they are needed.  This is how I tackle getting the hidden micro-rust off of the quarter.

Here is a close-up of the spots blasted with the Speed Blaster tool.

Here is a shot of the quarter after I have blasted all of the spots that showed the black ferric phosphate coating left on the surface of the hidden rust by the phosphoric acid.

After wiping the entire panel off with acetone, I treated the surface with phosphoric acid again to see what spots I might have missed.  Fortunately, there were only a few small spots that required a bit more blasting to completely remove the micro-rust that remained.

A final treatment with phosphoric acid Prep & Etch and the panel was ready for formal bodywork without the worry of having missed any hidden rust.
 

Thursday, January 9, 2014

Stripping the Rear Quarters and a Lesson to Share

Steady progress has been the order of the realm this past few weeks and I am quite happy with the ground that has been covered.  With a few new parts and tools added to the inventory, I had reached a point where it was time to get the rear quarter panels stripped of all remaining original paint to see what measures would be required to get them into a clean, rust-free bare metal state that would allow proper bodywork to proceed. 

Of the options available to remove paint from exterior surfaces of the body, I prefer chemical stripping over all other methods most of the time.  Chemical paint stripper is very easy to control, does an excellent job, and does not damage or alter the surface of the parent metal at all.  By using a razor blade scraper to skim the softened paint from the metal, the job of stripping an entire panel goes surprisingly quickly even with the “wait time” involved in letting the stripping chemical do its job.
After a short ceremony to pay homage to the last vestiges of medium metallic blue color that remained on the car, I applied the first coat of stripper using proper chemical resistant gloves, respirator and eye protection.  Allowing about 20 minutes for the surface coat to completely lift from the surface, I scraped the top layer of paint easily away from the surface with the razor scraper.  Generally speaking, this would leave the primer layer(s) on the surface that would simply require a second coat of stripper to remove completely.

Once all of the original paint and primer was completely removed, I rinsed the panels clean with distilled water on a shop towel to remove any stripper residue and neutralize the stripper.  The result was nice, bare metal panels that were ready for a close inspection and evaluation in order to begin planning the repair and prep work required to plan for primer and the sequence of conventional bodywork to come. 
The panel evaluation work is best accomplished without any sort of prep coatings or etchants on the panel so that even small details are not lost or masked.  This is particularly important on 40+ year old muscle cars as many manufacturers had not yet adopted immersion priming methods or anti-corrosion primers on all surfaces of the body.  EDP primers were still decades away before the last genuine muscle car rolled off the assembly line.  A close inspection is often remarkably enlightening as was the case here.  In fact, what I realized based on my inspection was I had a very unique opportunity to educate on the hidden evils that can exist under “survivor” original paint or older restoration work.  As such, the next section will cover this critical information with some very graphic examples of “what lies beneath” in more cases than you might imagine.
Aircraft stripper is a favorite of mine to chemically strip the last bit of factory paint from the rear quarters.  One thing to notice here is how relatively "rust free" the left rear quarter appears before the stripping work begins.

The first coat of chemical stripper very quickly starts to lift the original finish and is very easy to manage as evidenced by the lack of runoff of the stripper to the side of the quarter.

Nitrile gloves and an inexpensive razor scraper are an excellent combination for removing loosened layers of paint quickly and easily with relatively little mess.  I use a grout mixing tub to catch the debris for ease of clean up and to avoid crapping up my shop floor.

A bit closer look at the large curls of paint that are removed with the razor scraper.  Also note the remaining layer(s) of primer that will require a second coat of chemical stripper to remove.  Believe it or not, there is red oxide primer under the grey coating.

The top of the rear quarter has had its first round of chemical stripping complete and you can start seeing evidence of more extensive rust being exposed.  We will detail this discovery more in the second half of this article.

Moving to the front half of the quarter, the stripping process is identical and equally efficient.  A quick few minutes with the scraper and the second coat is applied over the same area and left to work for another 20 minute soak period.

After scraping off the second coat of stripper, the front half of the quarter is clean and down to bare metal.  Again, we see more evidence of the extent of surface rust that existed under the original paint and primer.

With all of the original paint and primer removed, the left rear quarter is completely exposed for a close inspection.

Moving to the right side quarter, the same stripping operation is applied.  In this shot, both the top and front half of the quarter has been completely stripped.

Here is an interesting detail that was revealed after the original paint and primer was stripped from the right rear quarter.  In the center of the picture, you can see where some sort of light sanding was done above the wheel arch at the factory before the car was painted.  It is not obvious what sort of flaw was being repaired, but 44 years ago, somebody thought it was important.
 
What You See Ain’t Always What You Get!

Nowadays, there is a tremendous amount of hype thrown around about preserving “original paint” as much as possible and avoiding stripping a car to bare metal during a restoration.  Well………bullshit.
Quite simply, with original paint left ANYWHERE on a body during restoration, you simply don’t what you don’t know because you can’t see what can’t be seen.  As it turns out, the rear quarters on the Boss were a perfect example in the most exemplary way.  If you look at the pictures below, you will see there are hints of what most describe as “minor surface rust” starting to peek out from the very weathered original paint.
As each layer of paint and primer starts to come off the panel during the stripping process, more and more evidence of surface rust starts to become exposed.  In fact, until the last trace of the base primer layer is completely gone, the full extent of the rust propagation is hard to imagine.  In fact, a general rule of thumb is that for every spec of rust you see perforating the surface of “original” paint, the extent of rust repair requirement is roughly 10-15 times larger in scale.  In other words, if you see a ¼” rust spot on the surface, the expected repair area will be approximately 2.5 to 3.75” across and often this can be a conservative estimate.
This simple fact is shown in undeniable and explicit detail in the following photographs of the tentacles of rust spreading widely across the panel that were completely hidden beneath the original finish.  Only until the panels were stripped to bare metal was the true extent of damage revealed.  Without this revelation, there is no way a proper assessment of the requisite repairs can be completed and any hope of a successful restoration of these surfaces is simply impossible.
With that, the lesson is to strip absolutely EVERYTHING to bare metal during a restoration to make absolutely sure the hundreds of hours of labor and untold thousands of dollars of investment you will make will be spent with maximum effect and long-term return.  It really is that important.
In the next update, I will document how to deal with the “ugliness” we have discovered.  Also, I will describe a simple process to reliably detect almost microscopic rust and how to eliminate it permanently.  Also, we will start getting into the repair of some small and moderate sized dents and dings.  Until the next update!
During the paint stripping process, the true extent of the surface rust propagation began to reveal itself.  In this close-up of the top of the left rear quarter, you can just start to see how the rust has extensive "tentacles" that extend far beyond the small spec that was revealed at the top of the painted surface.

A bit further rearward on the left quarter and this "rash" of rust became more and more visible as each layer of paint and primer were removed.  If you look closely, you will see a fair amount of primer is still left in the rusted area.

This is getting pretty ugly now.  After removing only the top layer of factory paint, the surface rust has been exposed and the true extent of coverage is pretty amazing.  Very quickly, it becomes obvious that the area that was originally visible is magnified many times over once we get all of the original paint and primer off the surfaces.
 
Pure ugliness.  Careful compare the detail in this photo to the one immediately above.  The speckles of rust here and there that were visible when we started have been revealed to be an extensive matrix of rust that extended all over the surface.  Roughly 75-80% of this rust was absolutely invisible on examination of the original paint!  Had I tried to preserve this finish in any way, the results in just a few years' time would be a total devastation of a very expensive paint job and likely the loss of the original panel.
 
With the top surfaces of the quarter stripped bare, you can clearly see why it is critical to avoid getting caught up in trying to save original paint in a full restoration.  What you can't see can definitely hurt you!